Freeze and Fuse with UGC Layering Mix

Demonstration on using UGC Layering Mix with powdered frit for making freeze & fuse glass. Here are a few places where you can purchase UGC Layering Mix. My schedule was as follows, but again, that's my kiln and maybe too conservative, due to lack of experience. COE96 It smells, so you want to vent to 800 400/1320/15 9999/950/60 300/100/0 Note: In addition to using colored frit, I have also tested with clear frit and then after firing, I have painted with enamel paint and put back into the kiln to fuse the paint to the glass (sintering) 350/1385/20 9999/950/30 100/700/0 one last note: I've also tested with the sludge that comes from my grinder. Scraped it up, sifted it and used it to make freeze and fuse pieces Unique Glass Colors https://www.uniqueglasscolors.com/ Colors for Earth https://colorsforearth.com Anything In Stained Glass https://www.anythinginstainedglass.co... If you have questions, you can reach me at [email protected]